Abstract:
This is an article in the field of metallurgical engineering. At the protection of argon gas, titanium-containing blast furnace slag produced titanium-silicon-aluminum alloy by aluminothermic reduction. The test result shows at 1 500 ℃, at the protection of argon gas, when aluminum powder accounts for 30%~40% of blast furnace slag, lime accounts for 5%~15% and fluorite ≥ 5%, the alloys obtained by reduction are mainly titanium-silicon phase, aluminum-silicon phase, titanium phases. In the alloy, the content of titanium, silicon, aluminum were 35%~40%, 26%~33%, 23%~32%, respectively. The recoveries of titanium, silicon, aluminum were 73%~88%, 84%~95%, 67%~77%, respectively.